Spatulate the Pulse paste opaque before applying. Use the Pulse paste
opaque liquid for dilution, if necessary.
Apply a full even layer of paste opaque to the framework and modify
with intensive opaques according to the desired chroma intensity.
In the case of non-precious alloys, it is recommended to use powder
opaque for the first opaque firing/ wash for the best results.
| Pulse
Press-To-Metal® (precious alloys)
|
| |
Start
Temp |
Closing
Time |
Start
Vacuum |
Temp.
Increase |
Final
Temp |
Hold
Time |
Cooling
Time |
| Degassing
|
400º
C |
1
min. |
* |
55-80ºC |
* |
* |
0 |
1st + 2nd Opaque
Firing |
400º C |
8 min. |
400º C |
55ºC |
950º C |
1 min |
0 |
|
Pulse
Press-To-Metal® (non-precious alloys)
|
| |
Start
Temp |
Closing
Time |
Start
Vacuum |
Temp.
Increase |
Final
Temp |
Hold
Time |
Cooling
Time |
| Degassing |
400º C |
1 min. |
* |
80ºC |
* |
* |
0 |
| Powder Opaque Firing |
400º C |
6 min. |
400º C |
55ºC |
980º C |
1 min |
0 |
| Paste Opaque
Firing |
400º C |
8 min. |
400º C |
55ºC |
950º C |
1 min |
0 |
|
* Please refer to the Alloy Manufacturer